Wood samples | Impregnation | Thermal treatment | Drying | r (%) | t (%) | a (%) | R (%) | 17E | NO | NO | SAC-30 | 3,90 | 9,84 | 0,85 | 14,58 | CpVI | NO | NO | DDS0.50 | 35,01 | 14,18 | 16,32 | 65,51 | DN5-BC | NO | NO | DDS0.50 | 33,52 | 23,72 | 14,19 | 71,44 | 2 E | NO | NO | SAC-40 | 2,15 | 12,65 | 0,19 | 14,99 | 3 E | NO | NO | SVC-30 | 11,22 | 23,15 | 7,05 | 41,42 | 3 E | NO | NO | SAC-30 | 18,18 | 17,37 | 6,73 | 42,28 | 4 E | NO | NO | SAC-30 | 7,32 | 10,71 | 3,08 | 21,11 | 5 E | NO | NO | SVC-30 | 0,93 | 10,56 | 0,18 | 11,67 | 5 E | NO | NO | SAC-40 | 7,50 | 8,71 | 1,17 | 17,38 | 6 E | NO | NO | SVC-30 | 3,70 | 11,67 | 0,61 | 15,98 | 7 E | NO | NO | SAC-40 | 15,54 | 14,37 | -1,67 | 28,25 | 7 E | NO | NO | SAC-30 | 15,84 | 14,25 | -1,65 | 28,44 | 7 E | NO | NO | SVC-30 | 10,21 | 23,44 | 3,22 | 36,88 | 7 E | NO | NO | SVC-30 | 11,26 | 25,47 | 5,67 | 42,40 | 8 E | NO | NO | SAC-40 | 2,96 | -0,50 | 1,11 | 3,57 | 9 E | NO | NO | SVC-30 | -1,10 | -13,04 | 1,72 | -12,42 | 9 E | NO | NO | SVC-20 | -10,57 | -1,07 | 0,36 | -11,28 | 10 E | NO | NO | SVC-30 | 4,97 | 11,92 | 4,48 | 21,37 | 11 E | NO | NO | SVC-30 | 6,98 | 6,65 | 5,17 | 18,80 | 12 E | NO | NO | DDS0.50 | 3,72 | 4,71 | 2,55 | 10,97 | 12 E | NO | NO | SAC-30 | 3,91 | 7,69 | 0,71 | 12,31 | 12 E | NO | NO | SAC-40 | 5,36 | 12,19 | -1,33 | 16,22 | 13 E | NO | NO | SAC-30 | 3,30 | 7,38 | -2,26 | 8,42 | 14 E | NO | NO | SVC-30 | -0,75 | 0,47 | -3,19 | -3,47 | 15 E | NO | NO | DDS0.50 | 10,00 | 7,96 | 0,85 | 18,80 | 15 E | NO | NO | SAC-40 | 17,46 | 7,82 | 0,00 | 25,28 | 15 E | NO | NO | SAC-40 | 17,46 | 7,69 | 1,11 | 26,26 | 16 E | NO | NO | SVC-30 | -6,60 | -30,13 | -0,01 | -36,74 | 18 E | NO | NO | SVC-40 | 2,75 | -1,27 | 1,84 | 3,32 | 18 E | NO | NO | SVC-20 | -14,10 | 16,67 | 0,85 | 3,42 | 18 E | NO | NO | DDS0.50 | 2,45 | 3,57 | 1,59 | 7,61 | 18 E | NO | NO | DDS0.50 | 10,45 | 9,32 | 1,67 | 21,44 | 18 E | NO | NO | SVC-30 | 8,33 | 16,67 | 0,85 | 25,85 | 18 E | NO | NO | SVC-40 | 10,20 | 16,22 | 1,28 | 27,70 |
Table 3: Shrinkage level (a: axial, r: radial, t: tangential) for different samples of waterlogged wood not impregnated, not thermally treated (NTT), dried with different techniques: - Dried by hot air (SAC - temperature °C) - Dried by continuous vacuum (SVC - temperature °C) - Dried by DDS (DDS - maximum pressure in bar).
|